Ra 1.6 is the most commonly specified surface finish on turned parts and the most commonly misunderstood. It can be produced by a finishing pass with a correctly chosen insert, by a polishing operation after turning, or by a tumbling process, and the three are not equivalent. A turned surface at Ra 1.6 carries a directional lay that a polished surface does not; a polished surface at the same Ra may have a different Rz and a different bearing ratio; and a tumbled surface may meet the number while rounding every edge on the part. Specifying CNC turning surface finish Ra without specifying how it is produced is specifying a number without specifying a surface.

Where the CNC Turning Surface Finish Ra Number Comes From
A turned surface is generated by a tool with a nose radius moving along the work at a feed rate. The geometry of that motion leaves a series of arcs, and the theoretical peak-to-valley height of those arcs is the feed squared divided by eight times the nose radius. A 0.1 mm per revolution feed with a 0.4 mm nose radius gives a theoretical height of about 3.1 microns, which corresponds to an Ra of roughly 0.4 microns. Change the feed to 0.2 mm per revolution and the height becomes 12.5 microns, with an Ra around 1.6.
That arithmetic is the whole reason Ra 1.6 is easy on a lathe: it is what a normal finishing feed produces with a normal insert. The number is not a precision achievement; it is the default result of cutting at 0.15 to 0.25 mm per revolution with a 0.4 to 0.8 mm nose radius. A shop that cannot hit Ra 1.6 by turning has a machine problem, a tool problem, or a rigidity problem, not a finishing problem.
The theoretical value is a floor, not a prediction. The actual surface is rougher because of vibration, built-up edge, tool wear, and the material’s tendency to tear rather than shear. On a stable machine with a sharp insert the actual is close to the theoretical; on a machine with a worn spindle bearing or a tool held too far out, the actual can be three times the theoretical and no amount of parameter adjustment will close the gap.
Ra Is One Number and the Surface Is Not
Ra is the arithmetic mean deviation of the profile from its mean line, and it is a single number that describes an average. Two surfaces with the same Ra can look and behave completely differently: one can be a uniform fine texture, the other a series of deep scratches separated by flat plateaus, and both average out to the same value. The parameter that distinguishes them is Rz, the average of the maximum peak-to-valley heights within the sampling length, and it is often the parameter that matters for sealing, wear, and fatigue.
The cut-off length is the second source of ambiguity. A profilometer measures over a sampling length and filters the profile with a cut-off, conventionally 0.8 mm for turned surfaces and 2.5 mm for rougher ones. The same surface measured with different cut-offs produces different Ra values, because a longer cut-off includes more of the waviness that a shorter one filters out. A drawing that specifies Ra without the cut-off has specified a number that two instruments will report differently.
The direction of measurement is the third. A turned surface has a lay — the helical direction of the feed marks — and Ra measured across the lay is different from Ra measured along it. The standard convention is to measure across the lay, because that is the direction the tool left the profile, and a measurement along the lay reads the smoothness of the individual feed mark rather than the roughness of the surface. A drawing that does not state the direction permits both, and the difference on a coarse turned surface can be a factor of two.
Turning Versus Polishing
Polishing removes the lay. A polished surface is isotropic: it has no directional texture, and its roughness comes from the abrasive rather than from a tool path. For a sealing face, an isotropic surface is usually better, because a directional lay can form a leak path along the marks. For a bearing surface, the lay direction matters and a turned surface with the lay running in the direction of motion is often superior to a polished one.
The cost difference is substantial. Turning to Ra 1.6 is a finishing pass that takes seconds. Polishing to Ra 1.6 is a manual or vibratory operation that takes minutes per part, adds a handling step, and introduces the risk of rounding edges and altering dimensions. On a part where the finish is cosmetic, polishing is an expensive way to meet a number that turning already meets. On a part where the finish is functional and the function requires isotropy, polishing is the correct process and the cost is justified.
The polishing vs turning decision therefore turns on function rather than on the Ra value. A hydraulic spool that must seal dynamically needs a specific lay and a specific Rz, and polishing may destroy the lay that makes it work. A cosmetic cover that must look uniform needs isotropy, and turning will leave a visible helix no matter how fine. The number is the same and the requirement is opposite.
| Route | Achievable Ra | Lay | Effect on edges and size | Cost |
|---|---|---|---|---|
| Finish turning, 0.15 mm/rev | 0.8 to 1.6 | Directional helix | None | 1.0 |
| Wiper insert, 0.3 mm/rev | 0.4 to 0.8 | Directional, flatter | None | 1.1 |
| Vibratory polish | 0.4 to 1.0 | Isotropic | Rounds edges 10 to 30 microns | 1.3 |
| Manual polish | 0.1 to 0.4 | Isotropic, operator dependent | Rounds edges, can alter size 5 to 20 microns | 2.4 |
The table makes the trade visible. The two turning routes cost almost nothing and deliver a directional surface with no dimensional consequence. The two polishing routes cost more and change the part: vibratory polishing rounds every edge by ten to thirty microns, which is fine on a deburred bracket and unacceptable on a part with a functional edge break, and manual polishing can move a diameter by twenty microns, which will fail a tight tolerance.
The Specification That Avoids the Argument
A complete surface specification has five parts: the parameter, the value, the cut-off, the direction, and the process if the process is constrained. “Ra 1.6, cut-off 0.8, measured across the lay, turned finish, no polishing” is a specification. “Ra 1.6” is a wish. The difference in cost between writing the first and writing the second is zero, and the difference in what arrives is substantial.
The process constraint is the part that buyers most often omit and most often need. A part that must be turned and not polished is a part where the lay direction matters, and saying so prevents a supplier from polishing to meet the number and destroying the function. A part that must be polished is a part where isotropy matters, and saying so prevents a supplier from turning to the number and leaving a helix.
The definitions behind these terms are standardised, and the ISO 4287 Ra definition sets out the parameters, the filters, and the evaluation length that the numbers refer to. Citing it on a drawing is not pedantry; it is the difference between a number that two inspectors measure the same way and a number that they do not.
Where Ra 1.6 Sits in Practice
Ra 1.6 is a general engineering finish. It is what a turned surface looks like when it is done properly, and it is adequate for most non-sealing, non-bearing surfaces. It is not adequate for a dynamic seal, which usually needs Ra 0.2 to 0.4 with a controlled Rz; it is not adequate for a bearing journal, which needs a specific Ra and a specific lay; and it is not adequate for an optical surface, which is a different order of specification entirely.
The most common error is specifying Ra 1.6 everywhere as a default. A drawing with a general note of Ra 1.6 and no individual symbols is a drawing that has applied a fine finish to every surface including the ones that do not need it, which adds a finishing pass to operations that could run at a rougher feed. The saving from removing that note from the non-functional surfaces is small per part and real across a production run.
The opposite error is specifying a finish only on the functional surface and leaving the rest undefined. An undefined surface defaults to whatever the process produces, which on a roughing pass can be Ra 6.3 or worse, and a rough surface on a non-functional area is a corrosion site, a fatigue initiation point, and a place where coating adhesion fails. The general note exists for a reason; the mistake is applying it to everything rather than to the surfaces where it matters.
The Feed Mark Is Not a Defect
Buyers new to turned parts sometimes reject a surface because they can see the helix, and the rejection is based on appearance rather than on measurement. A visible feed mark at Ra 1.6 is normal and expected; the eye resolves texture that the profilometer averages, and a surface that looks visibly turned can be entirely within a 1.6 specification. Rejecting on appearance without a measurement is the fastest way to a dispute that neither party can win, because there is no number to argue about.
The useful distinction is between a feed mark and a tear. A feed mark is regular, follows the tool path, and has a consistent pitch. A tear is irregular, follows the material’s grain, and appears as a smeared or torn patch rather than a helix. A tear is a defect and it indicates a dull tool, a built-up edge, or a material that is work-hardening. The two look similar in a photograph and completely different under a magnifier, and the difference is what a surface roughness turning specification is meant to control.
The second useful distinction is between roughness and waviness. Roughness is the fine texture within the sampling length; waviness is the longer undulation that the cut-off filters out. A surface can be smooth at Ra 0.8 and still be visibly wavy, and the waviness comes from vibration or from a machine geometry error rather than from the tool. A buyer who sees waves and specifies a tighter Ra will not fix the problem, because the Ra was already fine and the waves are at a different wavelength.
The practical answer is to specify both when both matter. A sealing face may need Ra 0.8 and a waviness limit; a cosmetic face may need only Ra. Specifying one and rejecting on the other is the most common form of finish dispute, and it is resolved by adding the second parameter rather than by tightening the first.
Where Coating Changes the Surface
Anodising, plating, and passivation all change the surface that was measured, and the change is not always in the direction the buyer expects. Anodising grows a conversion layer that follows the existing profile, so a turned surface anodised to fifteen microns is rougher after coating than before, because the coating reproduces the peaks and valleys at a slightly larger amplitude. A part specified at Ra 1.6 before anodising may read Ra 2.0 after, which is a rejection on a part that was conforming when it left the lathe.
Plating behaves differently. Zinc and nickel plating fill the valleys preferentially and can reduce Ra slightly, at the cost of building up on edges and in threads. Passivation removes a small amount of surface material and changes the chemistry rather than the profile, so the Ra is essentially unchanged and the corrosion resistance is not.
The specification has to say which state the finish applies to. “Ra 1.6 after anodising” is a requirement on the finished part and requires the machinist to produce a smoother surface than 1.6 to leave room for the coating. “Ra 1.6 before anodising” is a requirement on the machined part and permits the finished part to be rougher. The two are different products and the drawing usually says neither.
Measuring It, and Why the Measurement Disagrees
A profilometer with a diamond stylus dragged across the surface is the reference instrument, and its reading depends on the cut-off, the evaluation length, and the skid. A portable instrument held by hand on a curved surface reads differently from a bench instrument on a flat, because the skid follows the curvature and the stylus measures a combination of roughness and form. On a turned diameter, the measurement is usually taken along the axis with the skid supported, and the reading is only comparable if the setup is the same.
Optical instruments measure by interferometry or focus variation and produce a three-dimensional map rather than a traced line. They are faster, non-contacting, and better on soft or polished surfaces where a stylus would scratch, and their Ra values do not always agree with a stylus instrument because the sampling and filtering are different. A supplier and a customer using different instrument types will disagree by ten to twenty percent on the same surface, which is enough to fail a specification with no tolerance on the finish value.
The practical answer is to state the instrument or to accept a range. A specification of Ra 1.6 maximum measured by a stylus instrument with a 0.8 mm cut-off is checkable. A specification of Ra 1.6 with no instrument is a number that will be disputed at the first measurement, and the dispute will be about metrology rather than about the part.
The relationship between roughness and the geometry that produces it is the same one that governs form, and the vocabulary overlaps with this explanation of the difference between straightness and flatness, because a surface that is rough is also a surface whose form is harder to measure.
For a buyer, the useful question is not what Ra the supplier can achieve but which process will produce the surface and what that process does to the rest of the part. A turned Ra 1.6 changes nothing; a polished Ra 1.6 changes the edges and possibly the size. The CNC lathe services scope should state which finishes are produced by turning and which require a subsequent operation, because the two have different dimensional consequences and different prices.
The CNC turning parts manufacturer that asks which surfaces are functional before quoting a finish is a supplier that has understood the question. The one that quotes Ra 1.6 as a line item without asking is quoting a number, and the number will be met by whichever process is cheapest, which is not always the one the design needed.
A surface finish is not a value on a drawing. It is a description of a process, and the process determines whether the part seals, wears, or merely looks right. Ra 1.6 is easy; knowing which Ra 1.6 you need is the actual work.